These professional quality anodizing dyes provide consistent, quality results. The same dyes are sold to professional anodizing shops all over the world. 4oz of dye concentrate makes 2 Gallons.
These colors are approximate. The finish will normally have a more 'metallic' look, and will vary slightly depending on the alloy and surface preparation.
Procedure for Obtaining Dyed Anodize
Anodize the aluminum at 60-75°F for 90 minutes at 4.5 amps per sq foot or 0.03 amps per sq inch. Use our Anodizing Kit.
After thorough rinsing, immerse the part in the dye at a temperature of 140°F for 15 minutes.
Finally, seal by hanging the part in a sealer bath for 15 minutes.
All dyes are fully ROHS compliant.
            Safety Information
GHS Info
SDS
Product Videos
Product Reviews
13 Reviews Hide Reviews Show Reviews
- 
                
GOOD STAFF
GOOD STAFF
 - 
                
Hot rod red!
this is a beautiful red. Every time i take my parts out of it I'm in love with the color! Thanks!
 - 
                
Good products
Good products and fast shipping
 - 
                
Good product
Good product and fast shipping.
 - 
                
Good stuff!!!
Used as directed and parts came out really nice deep red . Surface prep is important as glassbead blasting gave it a matte finish . Will continue to order these fine products!!!
 - 
                
Nice true red
Great red color, pretty close match to Hornady red powder coat. One of the few dyes I do heat though as it takes a long time at room temp compared to my other dyes.
 - 
                
A real eye catcher, great red
Very desirable red, consistent results when used as instructed.
 - 
                
Blood Red
This color looks like a blood red color, not as bright as the color shown.
 - 
                
best red around
I love how well this red absorbs into the parts.
 
Important Information
Additional Equipment May Be Required
For Our Tank Plating Kits:
- Copper Pipe for tank bar
 - Copper Wire to hang items
 - Small amount of electrical wire to make connections
 - DC Power Supply - Included In Some Kits. Check kit contents on web site
 - Optional Rinse Tanks (or rinse over the plating tanks with a water bottle)
 - Other minor household items may be required, such as gloves, water etc.
 
For Our Anodizing Kits:
- DC Power Supply (Standard Kit Only)
 - 1 Gal Battery Acid
 - Dyes (if desired)
 - Optional Rinse Tanks (or rinse over the plating tanks with a water bottle)
 - Other minor household items may be required, such as gloves, water etc.
 
Learn More Before Buying
You can purchase our Caswell Plating Manual and learn how to use the kits, before purchasing a kit. Simply Order Here. When you are ready to buy, we will discount the price of the kit.
Already Have Our Plating Manual?
If you are ordering a plating kit that contains our Plating Manual, and you already have our Plating Manual, you can remove it from all kits that contain it and save $30 per kit. Just use Coupon Code NOMANUAL in your Shopping Cart at checkout.