Product Description
These professional quality anodizing dyes provide consistent, quality results. The same dyes are sold to professional anodizing shops all over the world. 4oz of dye concentrate makes 2 Gallons.
These colors are approximate. The finish will normally have a more 'metallic' look, and will vary slightly depending on the alloy and surface preparation.
Procedure for Obtaining Dyed Anodize
Anodize the aluminum at 60-75°F for 90 minutes at 4.5 amps per sq foot or 0.03 amps per sq inch. Use our Anodizing Kit.
After thorough rinsing, immerse the part in the dye at a temperature of 140°F for 15 minutes.
Finally, seal by hanging the part in a sealer bath for 15 minutes.
All dyes are fully ROHS compliant.

Safety Information
GHS Info

SDS
Product Videos
Product Reviews
24 Reviews Hide Reviews Show Reviews
-
Superior Product
Gives a great finish with deep, rich color and penetration. Works great with steam / boiling water sealing
-
Thanks for the prompt service
Very fast transaction and a great product
-
Best ever Anodixed
Anyone can do this perfectly with a few of these products and watch the videos on u tube.
-
new dye in the mix
Caswell has gone with a slightly different form of this dye. Instead of being liquid, this is in a powder form. You still mix it in the same quantity, just mix to distilled and heat. I'd have to say that I like it in powder form, although I question if it will remain unclumped like my last batch of black did to me. Looked like egg drop soup with black snot. I wasn't impressed. This however, seems to be working great.
-
black
Comes out a nice rich black. worked best for me when it was heated to 140 degrees.
-
you need it
It's black. Nothing more. It's probably the most used of any dye color. I do not like the price considering you use it so much and it does need to be replaced fairly frequently. But price and replacement factor doesn't affect the review.
Important Information
Additional Equipment May Be Required
For Our Tank Plating Kits:
- Copper Pipe for tank bar
- Copper Wire to hang items
- Small amount of electrical wire to make connections
- DC Power Supply - Included In Some Kits. Check kit contents on web site
- Optional Rinse Tanks (or rinse over the plating tanks with a water bottle)
- Other minor household items may be required, such as gloves, water etc.
For Our Anodizing Kits:
- DC Power Supply (Standard Kit Only)
- 1 Gal Battery Acid
- Dyes (if desired)
- Optional Rinse Tanks (or rinse over the plating tanks with a water bottle)
- Other minor household items may be required, such as gloves, water etc.
Learn More Before Buying
You can purchase our Caswell Plating Manual and learn how to use the kits, before purchasing a kit. Simply Order Here. When you are ready to buy, we will discount the price of the kit.
Already Have Our Plating Manual?
If you are ordering a plating kit that contains our Plating Manual, and you already have our Plating Manual, you can remove it from all kits that contain it and save $30 per kit. Just use Coupon Code NOMANUAL in your Shopping Cart at checkout.